Mountain Project Logo

Kalymnos Anchor Failure

John Byrnes · · Fort Collins, CO · Joined Dec 2007 · Points: 392

I think there's a lot of people who need to view this short video which was produced in 2010.  

The Thaitanium Project.  Notice all the commentary about how people denied the problem and how to fix it.

https://www.youtube.com/watch?v=af60D9EM-K4

Jim Titt · · Germany · Joined Nov 2009 · Points: 490
DrRockso RRG wrote:

Hey Greg, I was in the process of editing my post when you commented, I hadn’t read the whole thread yet or seen the Andy K photos. I’d be surprised to hear that the bolts themselves are all actually 316, or perhaps were sold as 316 but aren’t, I guess we’ll have to wait and see. The pictures for the one bolt seems like the head was getting absolutely eaten up by corrosion while the nut look more or less fine on the same bolt. Maybe hammering it in marred the surface. You would think they’d be seeing many more bolt failures on older routes bolted with 304, if even the 316 is experiencing failures.

Bad batches in marine grade stainless can be even worse than good quality 304, as we saw with fixe’s recalled first batch of PLX/HCR steel, which rusted even in arid environments.

It’s interesting that the (non stainless?) chain looks completely fine. Perhaps it was hot dipped galvanized. I recall a few areas where hot dipped galvanized eye bolts were the norm with good success due to the unavailability/cost prohibitive nature of titanium glue ins in their country.  

The hot-dipped forged iron bolts were manufactured and sold by the FFME (French federation) for many, many years. I've been to the factory where they were made, kinda cool, a bit like one of those medieval reenactment things but hot forging has always been like that. Not as cool as the blacksmith that makes the Sachsish sandstone bolts though!

DrRockso RRG · · Red River Gorge, KY · Joined Sep 2013 · Points: 1,414
John Byrnes wrote:

You better do a little research before calling me an armchair quarterback.   

Yes.  And in Thailand, Cuba, etc.  What makes you think that Kalymnos is special?   It's not.

I've been hearing that argument for 25 years.  Yawn.  Tired of it.

If you can't figure out how to rebolt them, ask nicely and I'll give you a hint.  It's not cheap.   And if you have shitty routes, don't rebolt them.  Remove the hangers from 1 and 2. No one will notice.

Good questions.  If they had developed the routes with titanium, THERE WOULD BE NO MAINTENANCE.  DUH!!   

I've rebolted something like three dozen routes on Cayman Brac myself and quarterbacked twice that many.  It's called work.  It's called money. It's called responsibility.  

I had this argument with the RRGCC twenty years ago too.   It's not the cost of the bolts, it's the recurring labor costs... that is, if you can get someone to do the labor and cough-up the money.  You guys made your bed, now you gotta sleep in it.

John, your comments were not the ones I was talking about with respect to armchair quarterbacking. It terms of "figuring out how to rebolt them" obviously there are ways to do this safely, (drilling temporary bolts ground up, etc) this is not a common practice for rebolting, though it may be necessary, which is why I brought it up. I was pointing out that things are not as easy as many would like to believe, there's already been one fatal accident from a corroded bolt failing on a reequipper. Care must be taken to ensure that folks are not putting themselves in grave danger doing the work. 

For some of these routes, simply climbing and setting a fixed line on the anchor or even weighting the anchor to haul up the drill could be hazard. I agree with your conclusion that the solution for some routes would be to simply close and unpublish them. Rebolt Kalymnos has already done a great job with messaging regarding not getting on routes with old sub-par hardware. 

To your point regarding using the proper materials, I agree, this is why having an LCO that buys and subsidizes then distributes the hardware for an area would help get the CORRECT hardware in to peoples hands.  

I'm curious who you spoke to at the RRGCC, the organization has never participated in the maintenance or purchase of any fixed hardware since its inception. I'm not sure if you're familiar with the program we've had going for the last 10+ years in the area, but through subsidizing and distributing high quality hardware, in the past 2 years alone over 400 routes have been developed, with near perfect compliance for developers using SS bolts, SS chain, and SS quicklinks. We've already been rebolting ONLY with SS glue-ins for last 15 years, I can't imagine anyone from the organization was arguing with you on sustainability and long term labor costs (at least no one involved now would), unless you were suggesting using only titanium for an area 600 miles inland from the nearest seawater.

BTW I love the plug for Titanium use in all coastal areas, I do think it's very worthwhile to investigate how 316 is performing in these areas, and how long can we expect the bolts that are already placed to last. It will greatly inform how the situation is managed, regardless of what is being used to replace bolts and develop new routes going forward.     

Greg Barnes · · American Safe Climbing Asso… · Joined Apr 2006 · Points: 3,797
Jim Titt wrote:

I've had deliveries of A2 bolts with A4 nuts, it just depends on what was available (it's normal that the bolt, nut and washer are from different grades and as long as the parts are all above the lowest allowed grade it's fine).

Makes sense, but they might have been A4 bolts too. It's not a good idea to assume anything - hopefully someone is testing them in a high quality and unbiased manner (if they even found all the broken bolts, I've searched for pieces & hangers many times at cliff bases, it's total luck whether you find them or not...).

Blake M · · Unknown Hometown · Joined Feb 2011 · Points: 1,869

While Jurassic Park isn't a super popular crag, I would hardly call it obscure, it was over 2k ticks on 8a and St Savvas seems to get logged a few times a year. 

Figuring out where to focus the limited rebolting resources does seem a bit tricky, if you only rebolt the popular routes then traffic gets even further condensed at already crowded areas. The real solution is probably more resources. Id bet that the vast majority of climbers have never given a cent to any sort of rebolting or crag maintenance. We as climbers need to be giving to and supporting reboting effors on a regular basis.

Nate Liles · · American Safe Climbing Asso… · Joined May 2012 · Points: 6

There has been extensive research into these materials outside of the climbing world in the aerospace, automotive, and industrial manufacturing industries, and it seems quite conclusive that 316/316L stainless steel is susceptible to microbiologically induced corrosion in Sulfate Reducing Bacteria (SRB) environments. This is not new information. Even as a layperson it seems quite clear that there is opportunity for these environments (even if quite rare) to exist on cliffs in certain regions.

SRB creates biofilms that produce corrosive sulfides, causing localized pitting and crevice corrosion, particularly in anaerobic conditions (this is a plausible explanation for why we see these attacks behind hangers and just below the rock surface), and it certainly seems like David Reeves hypothesis is a strong one here. 

With these mechanisms well documented, is any argument here for stainless bolts in these locations based on the fact that it is likely a rare set of conditions to be found in these climbing areas? Cost vs relatively low (but hard to predict) risk? Can we really tolerate that risk as a climbing community in the long term? Regardless of high cost, should we not change our new routing and rebolting standards to mandatory Ti in areas that have this risk so as to not dig ourselves a bigger hole for future rebolters?

climbkalymnos.com still lists local new routing standards as the following: "stainless steel bolts and hangers must always be used, i.e. 316L Marine or HCR expansion bolts, glue-in 316L Marine, HCR, or titanium expansion bolts using epoxy resin. All bolts must be certified by a manufacturer of climbing equipment. No homemade bolts, please."

Worth noting that in the most extreme environments, even Ti is not fully immune to these mechanisms, although it seems to have a far longer lifespan than other available options. I suppose Thailand will be our canary in a coal mine here...

It seems the situation in Kalymnos makes for a very long road ahead for the local climbing community. As someone who works very hard to keep my local crags well maintained for climbers, I cannot imagine being in this situation with a Russian roulette of bolts (thousands of them) needing attention, along with much of the local economy counting on visiting climbers.

Mr Rogers · · Pollock Pines and Bay area CA · Joined Aug 2010 · Points: 92

Article on SRB and Ti. I hadnt done too much digging into SRB and ti so this article was cool to dig into and open up a whole new time suck for myself to travel down.

Now, I think as Reeve points in some of his offerings to us, testing the rock in an area/crag is a good way to go about knowing if SRB will be likely or at incresed odds of effecting the hardware.

So spitballing here, it might be better to focus first on testing the rocks first, to know if that area should go under triage to replace all steel with Ti, or maybe that 316 will be super good enough and the re bolting effort can be done case by case.
IMO, new routes in sea side environmets should just use Ti as standard from this point going forward, as best practice is suggesting we should.
But testing allows the proverbial "we" to know what places to put energy into first.

David Reeve · · Unknown Hometown · Joined Jul 2020 · Points: 0
Mr Rogers wrote:

Article on SRB and Ti. I hadnt done too much digging into SRB and ti so this article was cool to dig into and open up a whole new time suck for myself to travel down.

Now, I think as Reeve points in some of his offerings to us, testing the rock in an area/crag is a good way to go about knowing if SRB will be likely or at incresed odds of effecting the hardware.

So spitballing here, it might be better to focus first on testing the rocks first, to know if that area should go under triage to replace all steel with Ti, or maybe that 316 will be super good enough and the re bolting effort can be done case by case.
IMO, new routes in sea side environmets should just use Ti as standard from this point going forward, as best practice is suggesting we should.
But testing allows the proverbial "we" to know what places to put energy into first.

Thanks for the reference. For some reason I have missed that one when searching for Ti - SRB research. A quick scan shows they have some electrochemistry in there - cool! Reading for a quiet time.

And as for "better to focus first on testing rocks....", you bet. At Kalymnos it has suddenly become absolutely critical to know if one has stumbled on a sulphate crag or not.

John Byrnes · · Fort Collins, CO · Joined Dec 2007 · Points: 392
David Reeve wrote:

Thanks for the reference. For some reason I have missed that one when searching for Ti - SRB research. A quick scan shows they have some electrochemistry in there - cool! Reading for a quiet time.

David, I have just a little information from 20 years ago about SRB corrosion and aluminum carabiners.  Some of the testing was done by Black Diamond and the rest by the UIAA. That is, if I can find it.  Perhaps some more quiet reading.  I think I still have the biners somewhere...

The short version is that bail biners left on bolts on Cayman Brac and elsewhere developed cracks that were identified as SCC before your research showed it was SRB.

And as for "better to focus first on testing rocks....", you bet. At Kalymnos it has suddenly become absolutely critical to know if one has stumbled on a sulphate crag or not.

Also 20 years ago I worked with the Access Fund Director (Robinson?) to come up with a guideline.  It went something like this, "If existing stainless steel bolts show any signs of corrosion or discoloration, new routes should use titanium."   That's crag specific, pretty simple and no testing required.

John Byrnes · · Fort Collins, CO · Joined Dec 2007 · Points: 392
Nate Liles wrote:

There has been extensive research into these materials outside of the climbing world in the aerospace, automotive, and industrial manufacturing industries, and it seems quite conclusive that 316/316L stainless steel is susceptible to microbiologically induced corrosion in Sulfate Reducing Bacteria (SRB) environments. This is not new information. Even as a layperson it seems quite clear that there is opportunity for these environments (even if quite rare) to exist on cliffs in certain regions.

SRB creates biofilms that produce corrosive sulfides, causing localized pitting and crevice corrosion, particularly in anaerobic conditions (this is a plausible explanation for why we see these attacks behind hangers and just below the rock surface), and it certainly seems like David Reeves hypothesis is a strong one here. 

With these mechanisms well documented, is any argument here for stainless bolts in these locations based on the fact that it is likely a rare set of conditions to be found in these climbing areas? Cost vs relatively low (but hard to predict) risk? Can we really tolerate that risk as a climbing community in the long term? Regardless of high cost, should we not change our new routing and rebolting standards to mandatory Ti in areas that have this risk so as to not dig ourselves a bigger hole for future rebolters?

climbkalymnos.com still lists local new routing standards as the following: "stainless steel bolts and hangers must always be used, i.e. 316L Marine or HCR expansion bolts, glue-in 316L Marine, HCR, or titanium expansion bolts using epoxy resin. All bolts must be certified by a manufacturer of climbing equipment. No homemade bolts, please."

What about titanium glue-in bolts with epoxy resin?  Duh.  Lost in translation...

Worth noting that in the most extreme environments, even Ti is not fully immune to these mechanisms, although it seems to have a far longer lifespan than other available options. I suppose Thailand will be our canary in a coal mine here...

It seems the situation in Kalymnos makes for a very long road ahead for the local climbing community. As someone who works very hard to keep my local crags well maintained for climbers, I cannot imagine being in this situation with a Russian roulette of bolts (thousands of them) needing attention, along with much of the local economy counting on visiting climbers.

Nate, I wish I could give your post about 100 "Thumbs Ups".   

I know there's some guys here on MP who have recent experience from Thailand, so can we hear from them about the state of their 25-year-old titanium bolts?   

I just got back from Cayman Brac and I can, without reservation, say the Ti bolts we placed in 2000 look brand new.  

John Byrnes · · Fort Collins, CO · Joined Dec 2007 · Points: 392
Greg Barnes wrote:

Makes sense, but they might have been A4 bolts too. It's not a good idea to assume anything - hopefully someone is testing them in a high quality and unbiased manner (if they even found all the broken bolts, I've searched for pieces & hangers many times at cliff bases, it's total luck whether you find them or not...).

This approach, testing before placing, isn't practical.  What are you gonna do?  Have the Customs guys test the bolts at the airport?  Therefore, it's essentially worthless.   

And besides, 316L fails too.    There's really only one safe choice.

Greg Barnes · · American Safe Climbing Asso… · Joined Apr 2006 · Points: 3,797
John Byrnes wrote:

This approach, testing before placing, isn't practical.  What are you gonna do?  Have the Customs guys test the bolts at the airport?  Therefore, it's essentially worthless.   

And besides, 316L fails too.    There's really only one safe choice.

There are a LOT of people who still insist that 316 is good enough and that all bolt failures were not 316. If they tested the bolt fragments from Kalymnos and found that they were 316, that would go a LONG way to help convince people that Ti is the only option.

As you know, the ASCA has been supplying 100% titanium glue-ins for any seaside bolt replacement for over 25 years, and supplied most of the bolts used for rebolting the popular crags in Thailand. California coast bolt failures were thought to be 316 (not 304) way back in the late '90s or 2000 or so, sometime before I helped Jim Thornburg replace a route with Ti glue-ins at Mickey's Beach in March 2001, and we've been getting titanium glue-ins to all coastal crags in the US since then (plus Thailand).

David Reeve · · Unknown Hometown · Joined Jul 2020 · Points: 0

There are a LOT of people who still insist that 316 is good enough and that all bolt failures were not 316. If they tested the bolt fragments from Kalymnos and found that they were 316, that would go a LONG way to help convince people that Ti is the only option.

I'm yet to find a verifiable example of SRB attack on 316, but I'll keep looking.

From a practical point of view, what matters, is the fact that we have plenty of examples of "apparent 316" failing under SRB attack. Remember that in the real world people are installing "apparent 316" and this, we know, can fail. I've pointed to testing with a magnet as a means of excluding a lot of fake 316. Certainly that helps, but in my experience, doesn't close the door.

I'm coming to the conclusion that it is actually less expensive to install titanium at a known sulphate crag than to ensure every piece of 316 you install is compliant. 

Kristian C · · Sheffield UK · Joined Mar 2024 · Points: 1

Although I don't live anywhere near the sea, this has prompted me out of curiosity to recheck the magnetic susceptibility of my stock of bolts and hardware. I have quite a wide selection from different well known manufactures. Previously I'd been using a weak mini horseshoe magnet. Now I also have a little but strong fridge magnet to test with. The little red fridge magnet in the photos is only just about holding its weight and in most cases could be easily flicked off. The larger magnet fails to stick to any of the items shown holding the red magnet.

The nut and washer on the wedge bolt were the only items that couldn't hold the small magnet but there is still some minute attraction.

Two bolts have a very strong attraction, enough to hold the heavier weak magnet. However neither of these are 316. The old Fixe bolt is some sort of PLX or whatever Fixe were using at the time. The polished twist bolt is apparently a special sea series bolt made from 1.4462 duplex stainless steel?

The question is are there any 316 products sold by climbing equipment manufacturers known to be non magnetic? Is this something to do with quality control of the bar stock coming in or has something changed once it has been worked? or is my mini fridge magnet so strong that you would expect a little bit of magnetic susceptibility in "good enough" 316?

Jim Titt · · Germany · Joined Nov 2009 · Points: 490

316 work-hardens (which makes it magnetic) if you bend or roll or similar, it's the way it is.

philip bone · · sonora · Joined Dec 2011 · Points: 15

I often see rust on the washer only on installed bolts of various vintage. Also, does the washer provide a moisture barrier? 

West slope Sierra Nevada 

Matt Sammons · · Tucson, AZ · Joined Sep 2019 · Points: 245
Jim Titt wrote:

316 work-hardens (which makes it magnetic) if you bend or roll or similar, it's the way it is.

Question for the metallurgical people out there. If true 316 stainless steel (e.g has high enough nickel and chromium) is worked and regains some magnetic properties, does that impact its resistance to oxidation, stress corrosion cracking or suffer reducing bacteria attack? 

My understanding is that it does not. 

In my work flow I use mostly 304ss, but have some 316ss (according the the label on the box, no independent testing to confirm). There is subtle difference in magnetic attraction between them. Huge difference in attraction between any ss variety and carbon/zinc plated steel you encounter on in-situ older hardware. I occasionally use this attribute to conform something is stainless vs non-stainless while rebolting. 

Re: original post topic - condolences to the Chech climbing committee and all impacted by the loss. Verified 316 or better (e.g. titanium) seems the only valid option for life supporting equipment in any area that can possibly be affected by such corrosion. 

Jim Titt · · Germany · Joined Nov 2009 · Points: 490
Matt Sammons wrote:

Question for the metallurgical people out there. If true 316 stainless steel (e.g has high enough nickel and chromium) is worked and regains some magnetic properties, does that impact its resistance to oxidation, stress corrosion cracking or suffer reducing bacteria attack? 

My understanding is that it does not. 

In my work flow I use mostly 304ss, but have some 316ss (according the the label on the box, no independent testing to confirm). There is subtle difference in magnetic attraction between them. Huge difference in attraction between any ss variety and carbon/zinc plated steel you encounter on in-situ older hardware. I occasionally use this attribute to conform something is stainless vs non-stainless while rebolting. 

Re: original post topic - condolences to the Chech climbing committee and all impacted by the loss. Verified 316 or better (e.g. titanium) seems the only valid option for life supporting equipment in any area that can possibly be affected by such corrosion. 

Dave Reeve wrote about this, it's very complicated though. He actualy uses a sensitive magnetic test to see how much martensite has formed. We also know that working it a low temperature has a negative effect but realistically this doesn't occur, I keep my workshop at over 16°C and the material as well. There also special welding rods which reduces the effect in welds but seeing a lot of the welding in climbjng bolts the rod is probably the least problem.

DrRockso RRG · · Red River Gorge, KY · Joined Sep 2013 · Points: 1,414
Matt Sammons wrote:

Question for the metallurgical people out there. If true 316 stainless steel (e.g has high enough nickel and chromium) is worked and regains some magnetic properties, does that impact its resistance to oxidation, stress corrosion cracking or suffer reducing bacteria attack? 

My understanding is that it does not. 

In my work flow I use mostly 304ss, but have some 316ss (according the the label on the box, no independent testing to confirm). There is subtle difference in magnetic attraction between them. Huge difference in attraction between any ss variety and carbon/zinc plated steel you encounter on in-situ older hardware. I occasionally use this attribute to conform something is stainless vs non-stainless while rebolting. 

Re: original post topic - condolences to the Chech climbing committee and all impacted by the loss. Verified 316 or better (e.g. titanium) seems the only valid option for life supporting equipment in any area that can possibly be affected by such corrosion. 

Yes, the change in microstructure from cold working will make the fixture marginally less corrosion resistant, and more prone to SCC/pitting corrosion since the metal is now holding internal stress and the surface is less uniform. Whether this marginal difference has any realistic difference whatsoever on climbing bolts in the wild, I don’t know. It seems a lot of the research points to the presence of SRB as a more compelling answer. Passivation and pickling or electro polishing can increase the corrosion resistance by cleaning/increasing the thickness of the passive layer on the surface of the bolt. Which can increase it’s longevity in certain environments but not make it immune to those conditions

A bolt being mildly magnetic is not a reliable test to figure out a grade of stainless, both 304 and 316 become mildly magnetic. With stainless vs zinc plated it’s typically abundantly obvious without need for a magnet to any trained eyed.

I think the question becomes how long is long enough. My personal take is that anything I’m  putting in the wall I’d like to last at least 50 years. 



John Byrnes · · Fort Collins, CO · Joined Dec 2007 · Points: 392

David Reeve wrote:

I'm yet to find a verifiable example of SRB attack on 316, but I'll keep looking.

In Angele Sjong's published, peer-reviewed analysis of a broken bolt hanger from Thailand, she quite clear that it is 316L.  Screenshot from her article.  Do you want a copy?

I'm coming to the conclusion that it is actually less expensive to install titanium at a known sulphate crag than to ensure every piece of 316 you install is compliant. 

Exactly correct.  

Guideline #1: Don't be a jerk.

Fixed Hardware: Bolts & Anchors
Post a Reply to "Kalymnos Anchor Failure"

Log In to Reply
Welcome

Join the Community! It's FREE

Already have an account? Login to close this notice.